MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Ineos TUB121GN High density bimodal polyethylene copolymer
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Pipe Grade

Material Notes: TUB121GN is a natural bimodal high density polyethylene copolymer designed for extrusion of potable water, natural gas, industrial and mining pipe. When blended with an approved black concentrate, the resulting formulation (“TUB121”) is listed by the Plastics Pipe Institute (PPI TR-4, as both PE 4710 and PE 100) and is certified to ANSI/NSF Standards 14 and 61, CSA B137.1 and CSA B137.4.

Information provided by INEOS

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.949 g/ccASTM D4883
Oxidative Induction Time (OIT) >= 20 min
@Temperature 210 °C
ASTM D3895
Melt Flow <= 0.10 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 0.24 g/10 min
@Load 5.00 kg,
Temperature 190 °C
ASTM D1238
 8.5 g/10 min
@Load 21.6 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
PENT >= 10000 hourASTM F1473
Hardness, Shore D 64ASTM D2240
Tensile Strength, Yield 24.1 MPa2 in/min.; ASTM D638
Elongation at Break >= 600 %2 in/min; ASTM D638
2% Secant Modulus 900 MPaASTM D790
Hydrostatic Design Basis 6.90 MPa
@Temperature 60.0 °C
Blended with approved black concentrate; ASTM D2837
 11.0 MPa
@Temperature 23.0 °C
Blended with approved black concentrate; ASTM D2837
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 126 °CASTM D1525
Brittleness Temperature <= -118 °CASTM D746
 
Descriptive Properties
Cell Classification445576CBlended with approved black concentrate. Contact INEOS Technical Service for a list of approved concentrates. ASTM D3350
Oxidative Resistance ClassificationCC3ASTM D3350
Thermal Stability (°C)> 240ASTM D3350

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PINEOS871 / 291477

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.