MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Syensqo (Solvay Specialty Polymers) Veradel® 3600 Polyethersulfone (PESU), Transparent
Categories: Polymer; Thermoplastic; Polyethersulfone (PES)

Material Notes: Transparent, very high melt flow for compounding

Veradel® 3600 is a very high melt flow general purpose amorphous PESU resin typically used for compounding glass and carbon fiber reinforced products. This transparent grade offers high heat deflection temperature, excellent toughness, dimensional stability and resistance to mineral acids. Other desirable properties include thermal stability, creep resistance and inherent flame resistance. Veradel® 3600 is FDA compliant and is approved for direct food contact. This grade was formerly marketed as Gafone™ PESU.

Applications: Compounding

Features: Acid Resistant; Chemical Resistant; Creep Resistant; Flame Retardant; Good Adhesion; Good Dimensional Stability; Good Thermal Stability; Good Toughness; High Flow; High Heat Resistance; High Tensile Strength; Hydrolysis Resistant; Low Molecular Weight; Medium Rigidity

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.37 g/ccASTM D792
 1.37 g/ccISO 1183
Water Absorption 0.50 %
@Time 86400 sec
ASTM D570
Linear Mold Shrinkage, Flow 0.0060 cm/cmASTM D955
Melt Flow 75 g/10 min
@Load 2.16 kg,
Temperature 380 °C
ASTM D1238
 75 g/10 min
@Load 2.16 kg,
Temperature 380 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 88.9 MPaASTM D638
Tensile Stress 90.0 MPaISO 527-2
Elongation at Break 30 %ISO 527-2
Elongation at Yield 6.5 %ASTM D638
 6.6 %ISO 527-2
Tensile Modulus 2690 MPaASTM D638
 2700 MPaISO 527-2
Flexural Strength 125 MPaASTM D790
 130 MPaISO 178
Flexural Modulus 2620 MPaASTM D790
 2750 MPaISO 178
Izod Impact, Notched 53.0 J/mASTM D256
Izod Impact, Notched (ISO) 5.60 kJ/m²ISO 180
Charpy Impact, Notched 6.00 kJ/m²ISO 179
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.70e+15 ohm-cmASTM D257
 1.70e+15 ohm-cmIEC 62631-3-1
Dielectric Constant 3.5
@Frequency 1000 Hz
ASTM D150
 3.51
@Frequency 60 Hz
ASTM D150
 3.54
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 15.0 kV/mm
@Thickness 3.00 mm
ASTM D149
 31.0 kV/mm
@Thickness 0.800 mm
IEC 60243-1
 31.0 kV/mm
@Thickness 0.800 mm
ASTM D149
Dissipation Factor 0.0017
@Frequency 60 Hz
ASTM D150
 0.0022
@Frequency 1000 Hz
ASTM D150
 0.0056
@Frequency 1e+6 Hz
ASTM D150
Comparative Tracking Index 125 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 52.0 µm/m-°CASTM D696
 52.0 µm/m-°CISO 11359-2
Deflection Temperature at 1.8 MPa (264 psi) 200 °CUnannealed, Injection Molded; ASTM D648
 203 °CUnannealed; ISO 75-2/A
UL RTI, Electrical 180 °C
@Thickness 3.00 mm
UL RTI, Mechanical with Impact 180 °C
@Thickness 3.00 mm
UL RTI, Mechanical without Impact 190 °C
@Thickness 3.00 mm
Flammability, UL94 V-0
@Thickness 1.50 mm
 
Processing PropertiesOriginal ValueComments
Zone 1 335 - 391 °CExtrusion
Zone 2 335 - 391 °CExtrusion
Zone 3 335 - 391 °CExtrusion
Zone 4 335 - 391 °CExtrusion
Zone 5 335 - 391 °CExtrusion
Adapter Temperature 327 - 371 °CExtrusion
Die Temperature 327 - 371 °CExtrusion
Melt Temperature 343 - 385 °CInjection
 343 - 391 °CExtrusion
Mold Temperature 149 - 163 °C
Drying Temperature 177 °C
@Time 9000 sec
 177 °C
@Time 9000 sec
Extrusion
 
Compliance PropertiesOriginal ValueComments
FDA Yes
 
Descriptive Properties
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
ColorTransparent - Slight Yellow
FormsPellets
Injection RateFast
ProcessingCompounding; Injection Molding
RoHS ComplianceYes
Screw Compression Ratio2.2:1.0

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSOL8Y4598 / 280398

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.