MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Domo TECHNYL® C 218 V50 BLACK PA 6 50% Glass Reinforced, Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 50% Glass Fiber Filled; Nylon 6, Heat Stabilized

Material Notes: Description: TECHNYL® C 218 V50 BLACK is a polyamide PA6, reinforced with 50% of glass fiber, heat stabilized, for injection molding. This product is available black.

Key Properties: High impact; Good surface aspect; Excellent thermal resistance

Benefits: This grade offers high mechanical strength, high surface aspect by easy flow & low pressure molding for injection molding. This grade offers high mechanical strength, high surface aspect by easy flow & low pressure molding for injection molding.

Applications: It is used in all sectors of industry, mainly for: Automotive parts, Housing and electrical sectors

DOMO Chemicals has acquired Solvay’s Performance Polyamides Business in Europe.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.56 g/ccISO 1183/A
Linear Mold Shrinkage, Flow 0.0030 cm/cm
Linear Mold Shrinkage, Transverse 0.0040 cm/cm
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 220 MPaASTM D638
 225 MPaISO 527 Type 1A
Elongation at Break 2.0 %ISO 527 Type 1A
 2.5 %ASTM D638
Tensile Modulus 14600 MPaISO 527 Type 1A
Flexural Strength 190 MPaASTM D790
Flexural Modulus 14000 MPaASTM D790
Izod Impact, Notched 19.4 kg-cm/cmASTM D256
Izod Impact, Notched (ISO) 17.0 kJ/m²ISO 180/1A
Charpy Impact Unnotched 107 kJ/m²ISO 179/1eU
Charpy Impact, Notched 19.0 kJ/m²ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmIEC 60093
Surface Resistance 1.00e+13 ohmIEC 60093
Dielectric Constant 3.8IEC 60250
Dissipation Factor 0.020IEC 60250
Comparative Tracking Index 550 VSol A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 22.0 µm/m-°C
@Temperature 23.0 - 85.0 °C
ISO 11359
Melting Point 222 °CISO 11357
Deflection Temperature at 1.8 MPa (264 psi) 215 °CASTM D648
 
Processing PropertiesOriginal ValueComments
Processing Temperature 240 - 250 °CCompression zone
 250 - 260 °CMixing zone
Feed Temperature 235 - 240 °C
Mold Temperature 60.0 - 90.0 °C
Drying Temperature 80.0 °C
Moisture Content <= 0.20 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSOLVAY861 / 218589

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.