MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Teknor Apex Monprene® WR-12250 CLR Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Monprene WR-12250 is a high performance clear thermoplastic elastomer designed for a variety of consumer application, including writing instrument requiring a soft, rubber-like feel. Monprene WR-12250 is a medium hardness, low density, lubricated, non-filled grade that exhibits excellent adhesion to PP for injection molding.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; Good Adhesion; Good Colorability; Good Flexibility; Good Moldability; Good Toughness; High Flow; Low Density; Medium Hardness; Low Specific Gravity; Lubricated; Slip; Without Fillers

Uses: Consumer Applications; Flexible Grips; Handles; Overmolding; Rubber Replacement; Soft Touch Applications; Writing Instruments

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding; Multi Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.890 g/ccASTM D792
Melt Flow 20 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 50
@Time 5.00 sec
Injection Molded; ASTM D2240
 52
@Time 1.00 sec
Injection Molded; ASTM D2240
Tensile Strength at Break 941 psiDie C, 20 in/min, Across Flow; ASTM D412
 1110 psiDie C, 20 in/min, Flow; ASTM D412
Tensile Stress at Strain 249 psi
@Strain 100 %
Die C, 20 in/min, Across Flow; ASTM D412
 317 psi
@Strain 100 %
Die C, 20 in/min, Flow; ASTM D412
 393 psi
@Strain 300 %
Die C, 20 in/min, Across Flow; ASTM D412
 460 psi
@Strain 300 %
Die C, 20 in/min, Flow; ASTM D412
Elongation at Break 630 %Die C, 20 in/min, Across Flow; ASTM D412
 690 %Die C, 20 in/min, Flow; ASTM D412
Tear Strength 159 pliDie C, 20 in/min, Across Flow; ASTM D624
 167 pliDie C, 20 in/min, Flow; ASTM D624
Compression Set 21 %
@Temperature 22.8 °C,
Time 79200 sec
Type 1; ASTM D395B
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 360 - 400 °F
Middle Barrel Temperature 360 - 400 °F
Front Barrel Temperature 360 - 400 °F
Nozzle Temperature 360 - 400 °F
Melt Temperature 360 - 400 °F
Mold Temperature 60.0 - 90.0 °F
Injection Pressure 200 - 800 psi
Back Pressure 25.0 - 100 psi
Cushion 0.150 - 1.00 in
Screw Speed 50 - 100 rpm
 
Descriptive Properties
AppearanceClear/Transparent

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PTEKNQ0970 / 237461

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.