MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Raschig Group 3535 Epoxy
Categories: Polymer; Thermoset; Epoxy; Epoxy, Molded, Glass Fiber Filler; Filled/Reinforced Thermoset

Material Notes: Glass fiber-reinforced epoxy molding compound. Good mechanical strength, very good electrical isolation properties adn dimensional stability even at high temperatures. Form: Low dust granulate packed in moisture resistant cartons, Standard carton size: 25 kg palletized in 750 kg loads. Processing: Compression/Transfer/Injection. Applications: Connectors, Thermocouples, Sensors, Resistors, Potentiometers.

Information provided by the Raschig Group

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.90 - 2.10 g/ccISO 1183
Apparent Bulk Density 0.850 - 1.00 g/ccISO 60
Water Absorption <= 0.10 %
@Temperature 23.0 °C,
Time 86400 sec
ISO 62
Linear Mold Shrinkage 0.0030 - 0.0050 cm/cm(longitudinal) Injection and Compression; ISO 2577
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 60.0 - 70.0 MPaInjection and Compression; ISO 527
Modulus of Elasticity 15.0 - 18.0 GPaInjection and Compression; ISO 527
Flexural Strength 120 - 140 MPaInjection and Compression; ISO 178
Flexural Modulus 14.0 - 16.0 GPaInjection and Compression; ISO 178
Compressive Strength 150 - 200 MPaISO 604
Charpy Impact Unnotched 0.800 - 1.20 J/cm²
@Temperature 23.0 °C
Injection and Compression; ISO 179/ 1eU
Charpy Impact, Notched 0.250 - 0.350 J/cm²
@Temperature 23.0 °C
Injection and Compression; ISO 179/ 1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 - 1.00e+16 ohm-cmIEC 60093
Surface Resistance 1.00e+14 - 1.00e+15 ohmIEC 60093
Dielectric Constant 4.0 - 6.0
@Frequency 1e+6 Hz
IEC 60250
 5.0 - 7.0
@Frequency 100 Hz
IEC 60250
Dielectric Strength 15.0 - 20.0 kV/mm
@Thickness 1.00 mm
IEC 60243-1
Dissipation Factor 0.010 - 0.030
@Frequency 100 Hz
IEC 60250
 0.010 - 0.030
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index >= 250 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear 15.0 - 20.0 µm/m-°C
@Temperature 50.0 - 150 °C
ISO 11359-2
Thermal Conductivity 0.600 - 0.800 W/m-KASTM E1461
Deflection Temperature at 1.8 MPa (264 psi) >= 200 °CInjection; ISO 75-A
Deflection Temperature at 8.0 MPa 170 - 190 °CInjection; ISO 75-C
Flammability, UL94 V-0
@Thickness 5.70 mm
Shrinkage <= 0.050 %
@Temperature 110 °C,
Time 605000 sec
Post-shrinkage; ISO 2577
 
Processing PropertiesOriginal ValueComments
Shelf Life 6.00 Month
@Temperature 15.0 - 25.0 °C
 
Descriptive Properties
Arc Resistance4 StufeASTM D495
Glow wire flammability test900/1IEC 60695 2-12
Glow wire ignitability test900/1IEC 60695 2-13
Water Absorption<10 mgISO 62; 24h / 23°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Hexcel® F161 Epoxy Resin, 120 Glass Fabric
Raschig Group EPOXIDUR® 3585 EP Epoxy, Molded, Glass Fiber Filler
Tisan TISAKRIL® 15% Glass Fiber Reinforced ABS
Cotronics Duralco™ 4703 Adhesive and Tooling Compound
Cotronics Duralco™ 4460 Electrically Resistant, Low Viscosity Epoxy Adhesive, Coating, and Sealant

PRASCH15 / 65300

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.