MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Toyobo GLAMIDE® T-662 Nylon-66
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Unreinforced, Flame Retardant

Material Notes: GLAMIDE® is very tough and exhibits high abrasion resistance. It has a high melting point and heat resistance, has well-balanced proportions of mechanical properties, performs self-distinguishing and a specific grade approved as UL94V-0 class is provided, and it exhibits excellent chemical resistance and oil resistance. Grade T-662 is a standard type, non-reinforced Nylon-66.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.14 g/ccAbsolute Drying; ASTM-D792
Water Absorption 1.2 %Absolute Drying; ASTM-D570
Moisture Absorption at Equilibrium 2.5 %Absolute Drying; ASTM-D570
Linear Mold Shrinkage 0.0060 - 0.012 cm/cm
@Thickness 1.00 mm
Absolute Drying
 0.015 - 0.022 cm/cm
@Thickness 3.00 mm
Absolute Drying
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 120Absolute Drying; ASTM-D785
Tensile Strength, Ultimate 28.0 MPa
@Temperature 80.0 °C
Practical Use (Water Absorption 2.5%); ASTM-D638
 38.0 MPa
@Temperature 80.0 °C
Absolute Drying; ASTM-D638
 50.0 MPa
@Temperature 23.0 °C
Practical Use (Water Absorption 2.5%); ASTM-D638
 82.0 MPa
@Temperature 23.0 °C
Absolute Drying; ASTM-D638
 110 MPa
@Temperature -40.0 °C
Practical Use (Water Absorption 2.5%); ASTM-D638
 116 MPa
@Temperature -40.0 °C
Absolute Drying; ASTM-D638
Elongation at Break 120 %Absolute Drying; ASTM-D638
 >= 200 %Practical Use (Water Absorption 2.5%); ASTM-D638
Flexural Strength 40.0 MPa
@Temperature 80.0 °C
Practical Use (Water Absorption 2.5%); ASTM-D790
 66.0 MPa
@Temperature 23.0 °C
Practical Use (Water Absorption 2.5%); ASTM-D790
 66.0 MPa
@Temperature 80.0 °C
Absolute Drying; ASTM-D790
 117 MPa
@Temperature 23.0 °C
Absolute Drying; ASTM-D790
 120 MPa
@Temperature -40.0 °C
Practical Use (Water Absorption 2.5%); ASTM-D790
 140 MPa
@Temperature -40.0 °C
Absolute Drying; ASTM-D790
Flexural Modulus 0.600 GPa
@Temperature 80.0 °C
Practical Use (Water Absorption 2.5%); ASTM-D790
 1.00 GPa
@Temperature 80.0 °C
Absolute Drying; ASTM-D790
 1.40 GPa
@Temperature 23.0 °C
Practical Use (Water Absorption 2.5%); ASTM-D790
 2.90 GPa
@Temperature 23.0 °C
Absolute Drying; ASTM-D790
 4.00 GPa
@Temperature -40.0 °C
Practical Use (Water Absorption 2.5%); ASTM-D790
 4.30 GPa
@Temperature -40.0 °C
Absolute Drying; ASTM-D790
Compressive Strength 90.0 MPaAbsolute Drying; ASTM-D695
Izod Impact, Notched 35.0 J/m
@Temperature -40.0 °C
Absolute Drying; ASTM-D256
 40.0 J/m
@Temperature -40.0 °C
Practical Use (Water Absorption 2.5%); ASTM-D256
 45.0 J/m
@Temperature 23.0 °C
Absolute Drying; ASTM-D256
 300 J/m
@Temperature 23.0 °C
Practical Use (Water Absorption 2.5%); ASTM-D256
Taber Abrasion, mg/1000 Cycles 8.0CS-17, Absolute Drying; ASTM-D1044
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+9 - 1.00e+10 ohm-cmPractical Use (Water Absorption 2.5%); ASTM-D257
 1.00e+12 ohm-cmAbsolute Drying; ASTM-D257
Dielectric Constant 3.9
@Frequency 1000 Hz
Absolute Drying; ASTM-D150
 6.5
@Frequency 1000 Hz
Practical Use (Water Absorption 2.5%); ASTM-D150
Dielectric Strength 13.0 kV/mm
@Thickness 2.00 mm
Practical Use (Water Absorption 2.5%); ASTM-D149
 20.0 kV/mm
@Thickness 2.00 mm
Absolute Drying; ASTM-D149
Arc Resistance 110 secPractical Use (Water Absorption 2.5%); ASTM-D495
 120 secAbsolute Drying; ASTM-D495
Comparative Tracking Index >= 600 VIEC Method
 
Thermal PropertiesOriginal ValueComments
CTE, linear 80.0 µm/m-°CAbsolute Drying; ASTM-D696
Deflection Temperature at 0.46 MPa (66 psi) 230 °CAbsolute Drying; ASTM-D648
Deflection Temperature at 1.8 MPa (264 psi) 80.0 °CAbsolute Drying; ASTM-D648
Flammability, UL94 HB
 
Processing PropertiesOriginal ValueComments
Melt Temperature 270 - 290 °C
Mold Temperature 40.0 - 80.0 °C
Injection Pressure 30.0 - 40.0 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aardvark Polymers Aarlon® 4055FR PA 6/6 Rotational Molding Resin
Zell-Metall Engineering Plastics Zellamid 250 (PA6.6)

PTOY914 / 107465

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.