Physical Properties | Original Value | Comments |
---|
Density | 2.83 g/cc |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Brinell | 140 |
Hardness, Knoop | 177 |
Hardness, Rockwell A | 51.6 |
Hardness, Rockwell B | 84 |
Hardness, Vickers | 162 |
Tensile Strength, Ultimate | 510 MPa @Temperature 24.0 °C |
| 117 MPa @Temperature 204 °C, Time 3.60e+7 sec |
| 131 MPa @Temperature 204 °C, Time 3.60e+6 sec |
| 159 MPa @Temperature 177 °C, Time 3.60e+7 sec |
| 165 MPa @Temperature 204 °C, Time 360000 sec |
| 193 MPa @Temperature 177 °C, Time 3.60e+6 sec |
| 221 MPa @Temperature 149 °C, Time 3.60e+7 sec |
| 221 MPa @Temperature 204 °C, Time 36000 sec |
| 248 MPa @Temperature 177 °C, Time 360000 sec |
| 290 MPa @Temperature 149 °C, Time 3.60e+6 sec |
| 290 MPa @Temperature 204 °C, Time 1800 sec |
| 303 MPa @Temperature 204 °C, Time 360 sec |
| 324 MPa @Temperature 177 °C, Time 36000 sec |
| 352 MPa @Temperature 177 °C, Time 1800 sec |
| 359 MPa @Temperature 149 °C, Time 360000 sec |
| 359 MPa @Temperature 177 °C, Time 360 sec |
| 393 MPa @Temperature 149 °C, Time 1800 sec |
| 393 MPa @Temperature 149 °C, Time 36000 sec |
| 393 MPa @Temperature 149 °C, Time 360 sec |
| 441 MPa @Temperature 100 °C, Time 360 - 36000 sec |
| 441 MPa @Temperature 100 °C, Time 3.60e+6 sec |
| 441 MPa @Temperature 100 °C, Time 3.60e+7 sec |
| 448 MPa @Temperature 100 °C, Time 360000 sec |
| 510 MPa @Treatment Temp. 24.0 °C |
| 234 MPa @Treatment Temp. 204 °C, Time 3.60e+7 sec |
| 248 MPa @Treatment Temp. 177 °C, Time 3.60e+7 sec |
| 262 MPa @Treatment Temp. 204 °C, Time 3.60e+6 sec |
| 317 MPa @Treatment Temp. 177 °C, Time 3.60e+6 sec |
| 317 MPa @Treatment Temp. 204 °C, Time 360000 sec |
| 331 MPa @Treatment Temp. 149 °C, Time 3.60e+7 sec |
| 386 MPa @Treatment Temp. 177 °C, Time 360000 sec |
| 386 MPa @Treatment Temp. 204 °C, Time 36000 sec |
| 407 MPa @Treatment Temp. 149 °C, Time 3.60e+6 sec |
| 469 MPa @Treatment Temp. 177 °C, Time 36000 sec |
| 469 MPa @Treatment Temp. 204 °C, Time 1800 sec |
| 483 MPa @Treatment Temp. 149 °C, Time 360000 sec |
| 490 MPa @Treatment Temp. 204 °C, Time 360 sec |
| 496 MPa @Treatment Temp. 177 °C, Time 1800 sec |
| 503 MPa @Treatment Temp. 149 °C, Time 36000 sec |
| 510 MPa @Treatment Temp. 100 °C, Time 3.60e+7 sec |
| 510 MPa @Treatment Temp. 149 °C, Time 360 sec |
| 510 MPa @Treatment Temp. 149 °C, Time 1800 sec |
| 510 MPa @Treatment Temp. 177 °C, Time 360 sec |
| 510 MPa @Treatment Temp. 100 °C, Time 360 - 36000 sec |
| 510 MPa @Treatment Temp. 100 °C, Time 360000 sec |
| 510 MPa @Treatment Temp. 100 °C, Time 3.60e+6 sec |
Tensile Strength, Yield | 455 MPa @Temperature 24.0 °C |
| 90.0 MPa @Temperature 204 °C, Time 3.60e+7 sec |
| 110 MPa @Temperature 204 °C, Time 3.60e+6 sec |
| 124 MPa @Temperature 177 °C, Time 3.60e+7 sec |
| 152 MPa @Temperature 204 °C, Time 360000 sec |
| 172 MPa @Temperature 177 °C, Time 3.60e+6 sec |
| 193 MPa @Temperature 149 °C, Time 3.60e+7 sec |
| 207 MPa @Temperature 204 °C, Time 36000 sec |
| 234 MPa @Temperature 177 °C, Time 360000 sec |
| 276 MPa @Temperature 149 °C, Time 3.60e+6 sec |
| 276 MPa @Temperature 204 °C, Time 1800 sec |
| 290 MPa @Temperature 204 °C, Time 360 sec |
| 310 MPa @Temperature 177 °C, Time 36000 sec |
| 332 MPa @Temperature 149 °C, Time 360000 sec |
| 345 MPa @Temperature 177 °C, Time 360 sec |
| 345 MPa @Temperature 177 °C, Time 1800 sec |
| 386 MPa @Temperature 149 °C, Time 360 sec |
| 386 MPa @Temperature 149 °C, Time 1800 sec |
| 386 MPa @Temperature 149 °C, Time 36000 sec |
| 421 MPa @Temperature 100 °C, Time 3.60e+7 sec |
| 427 MPa @Temperature 100 °C, Time 360 - 36000 sec |
| 427 MPa @Temperature 100 °C, Time 3.60e+6 sec |
| 434 MPa @Temperature 100 °C, Time 360000 sec |
| 455 MPa @Treatment Temp. 24.0 °C |
| 117 MPa @Treatment Temp. 204 °C, Time 3.60e+7 sec |
| 138 MPa @Treatment Temp. 204 °C, Time 3.60e+6 sec |
| 152 MPa @Treatment Temp. 177 °C, Time 3.60e+7 sec |
| 200 MPa @Treatment Temp. 204 °C, Time 360000 sec |
| 214 MPa @Treatment Temp. 177 °C, Time 3.60e+6 sec |
| 228 MPa @Treatment Temp. 149 °C, Time 3.60e+7 sec |
| 283 MPa @Treatment Temp. 204 °C, Time 36000 sec |
| 296 MPa @Treatment Temp. 177 °C, Time 360000 sec |
| 317 MPa @Treatment Temp. 149 °C, Time 3.60e+6 sec |
| 400 MPa @Treatment Temp. 177 °C, Time 36000 sec |
| 407 MPa @Treatment Temp. 149 °C, Time 360000 sec |
| 421 MPa @Treatment Temp. 204 °C, Time 1800 sec |
| 434 MPa @Treatment Temp. 204 °C, Time 360 sec |
| 441 MPa @Treatment Temp. 100 °C, Time 3.60e+7 sec |
| 441 MPa @Treatment Temp. 149 °C, Time 36000 sec |
| 441 MPa @Treatment Temp. 177 °C, Time 1800 sec |
| 448 MPa @Treatment Temp. 149 °C, Time 1800 sec |
| 448 MPa @Treatment Temp. 177 °C, Time 360 sec |
| 455 MPa @Treatment Temp. 100 °C, Time 360 - 36000 sec |
| 455 MPa @Treatment Temp. 100 °C, Time 3.60e+6 sec |
| 455 MPa @Treatment Temp. 149 °C, Time 360 sec |
| 462 MPa @Treatment Temp. 100 °C, Time 360000 sec |
Elongation at Break | 11 % @Temperature 24.0 °C |
| 13 % @Temperature 100 °C, Time 360 - 36000 sec |
| 13 % @Temperature 100 °C, Time 360000 sec |
| 14 % @Temperature 100 °C, Time 3.60e+6 sec |
| 15 % @Temperature 100 °C, Time 3.60e+7 sec |
| 16 % @Temperature 149 °C, Time 360 sec |
| 17 % @Temperature 149 °C, Time 1800 sec |
| 18 % @Temperature 149 °C, Time 36000 sec |
| 19 % @Temperature 149 °C, Time 360000 sec |
| 19 % @Temperature 177 °C, Time 360 sec |
| 20 % @Temperature 177 °C, Time 1800 sec |
| 21 % @Temperature 149 °C, Time 3.60e+6 sec |
| 22 % @Temperature 177 °C, Time 36000 sec |
| 22 % @Temperature 204 °C, Time 360 sec |
| 23 % @Temperature 204 °C, Time 1800 sec |
| 25 % @Temperature 177 °C, Time 360000 sec |
| 27 % @Temperature 204 °C, Time 36000 sec |
| 29 % @Temperature 149 °C, Time 3.60e+7 sec |
| 31 % @Temperature 177 °C, Time 3.60e+6 sec |
| 32 % @Temperature 204 °C, Time 360000 sec |
| 40 % @Temperature 177 °C, Time 3.60e+7 sec |
| 45 % @Temperature 204 °C, Time 3.60e+6 sec |
| 54 % @Temperature 204 °C, Time 3.60e+7 sec |
| 11 % @Treatment Temp. 24.0 °C |
| 11 % @Treatment Temp. 100 °C, Time 360 - 36000 sec |
| 11 % @Treatment Temp. 149 °C, Time 360 sec |
| 12 % @Treatment Temp. 100 °C, Time 360000 sec |
| 12 % @Treatment Temp. 100 °C, Time 3.60e+6 sec |
| 12 % @Treatment Temp. 100 °C, Time 3.60e+7 sec |
| 12 % @Treatment Temp. 149 °C, Time 1800 sec |
| 12 % @Treatment Temp. 149 °C, Time 36000 sec |
| 12 % @Treatment Temp. 177 °C, Time 360 sec |
| 12 % @Treatment Temp. 177 °C, Time 1800 sec |
| 12 % @Treatment Temp. 204 °C, Time 360 sec |
| 12 % @Treatment Temp. 204 °C, Time 1800 sec |
| 13 % @Treatment Temp. 149 °C, Time 360000 sec |
| 13 % @Treatment Temp. 149 °C, Time 3.60e+6 sec |
| 13 % @Treatment Temp. 177 °C, Time 36000 sec |
| 13 % @Treatment Temp. 177 °C, Time 360000 sec |
| 13 % @Treatment Temp. 204 °C, Time 36000 sec |
| 14 % @Treatment Temp. 149 °C, Time 3.60e+7 sec |
| 14 % @Treatment Temp. 177 °C, Time 3.60e+6 sec |
| 14 % @Treatment Temp. 204 °C, Time 360000 sec |
| 15 % @Treatment Temp. 177 °C, Time 3.60e+7 sec |
| 16 % @Treatment Temp. 204 °C, Time 3.60e+6 sec |
| 19 % @Treatment Temp. 204 °C, Time 3.60e+7 sec |
Creep Strength | 124 MPa @Temperature 149 °C, Time 3.60e+6 sec |
| 145 MPa @Temperature 149 °C, Time 3.60e+6 sec |
| 152 MPa @Temperature 149 °C, Time 360000 sec |
| 165 MPa @Temperature 149 °C, Time 3.60e+6 sec |
| 179 MPa @Temperature 149 °C, Time 3.60e+6 sec |
| 193 MPa @Temperature 149 °C, Time 360000 sec |
| 228 MPa @Temperature 149 °C, Time 36000 sec |
| 241 MPa @Temperature 149 °C, Time 360000 sec |
| 255 MPa @Temperature 149 °C, Time 360000 sec |
| 269 MPa @Temperature 149 °C, Time 36000 sec |
| 290 MPa @Temperature 149 °C, Time 36000 sec |
| 290 MPa @Temperature 149 °C, Time 3600 sec |
| 303 MPa @Temperature 149 °C, Time 36000 sec |
| 303 MPa @Temperature 149 °C, Time 3600 sec |
| 317 MPa @Temperature 100 °C, Time 3.60e+6 sec |
| 324 MPa @Temperature 149 °C, Time 3600 sec |
| 324 MPa @Temperature 149 °C, Time 360 sec |
| 331 MPa @Temperature 100 °C, Time 360000 sec |
| 338 MPa @Temperature 149 °C, Time 3600 sec |
| 345 MPa @Temperature 100 °C, Time 3.60e+6 sec |
| 345 MPa @Temperature 100 °C, Time 360000 sec |
| 345 MPa @Temperature 149 °C, Time 360 sec |
| 352 MPa @Temperature 100 °C, Time 3.60e+6 sec |
| 359 MPa @Temperature 149 °C, Time 360 sec |
| 359 MPa @Temperature 100 °C, Time 36000 sec |
| 365 MPa @Temperature 149 °C, Time 360 sec |
| 365 MPa @Temperature 100 °C, Time 360000 sec |
| 372 MPa @Temperature 100 °C, Time 360000 sec |
| 372 MPa @Temperature 100 °C, Time 36000 sec |
| 386 MPa @Temperature 100 °C, Time 36000 sec |
| 386 MPa @Temperature 100 °C, Time 3600 sec |
| 393 MPa @Temperature 100 °C, Time 36000 sec |
| 400 MPa @Temperature 100 °C, Time 3600 sec |
| 407 MPa @Temperature 100 °C, Time 3600 sec |
| 414 MPa @Temperature 100 °C, Time 3600 sec |
| 414 MPa @Temperature 100 °C, Time 360 sec |
| 421 MPa @Temperature 100 °C, Time 360 sec |
| 427 MPa @Temperature 100 °C, Time 360 sec |
| 434 MPa @Temperature 100 °C, Time 360 sec |
| 434 MPa @Temperature 24.0 °C, Time 360000 sec |
| 441 MPa @Temperature 24.0 °C, Time 3.60e+6 sec |
| 441 MPa @Temperature 24.0 °C, Time 36000 sec |
| 441 MPa @Temperature 24.0 °C, Time 360000 sec |
| 441 MPa @Temperature 24.0 °C, Time 3600 sec |
| 441 MPa @Temperature 24.0 °C, Time 36000 sec |
| 448 MPa @Temperature 24.0 °C, Time 3.60e+6 sec |
| 448 MPa @Temperature 24.0 °C, Time 360000 sec |
| 448 MPa @Temperature 24.0 °C, Time 3600 sec |
| 448 MPa @Temperature 24.0 °C, Time 360 sec |
| 455 MPa @Temperature 24.0 °C, Time 360000 sec |
| 455 MPa @Temperature 24.0 °C, Time 36000 sec |
| 455 MPa @Temperature 24.0 °C, Time 360 sec |
| 462 MPa @Temperature 24.0 °C, Time 3600 sec |
| 469 MPa @Temperature 24.0 °C, Time 36000 sec |
| 476 MPa @Temperature 24.0 °C, Time 360 sec |
| 483 MPa @Temperature 24.0 °C, Time 3600 sec |
| 496 MPa @Temperature 24.0 °C, Time 360 sec |
Rupture Strength | 179 MPa @Temperature 149 °C, Time 3.60e+6 sec |
| 262 MPa @Temperature 149 °C, Time 360000 sec |
| 310 MPa @Temperature 149 °C, Time 36000 sec |
| 345 MPa @Temperature 149 °C, Time 3600 sec |
| 359 MPa @Temperature 100 °C, Time 3.60e+6 sec |
| 372 MPa @Temperature 149 °C, Time 360 sec |
| 379 MPa @Temperature 100 °C, Time 360000 sec |
| 407 MPa @Temperature 100 °C, Time 36000 sec |
| 427 MPa @Temperature 100 °C, Time 3600 sec |
| 441 MPa @Temperature 100 °C, Time 360 sec |
| 469 MPa @Temperature 24.0 °C, Time 3.60e+6 sec |
| 476 MPa @Temperature 24.0 °C, Time 360000 sec |
| 490 MPa @Temperature 24.0 °C, Time 36000 sec |
| 503 MPa @Temperature 24.0 °C, Time 3600 sec |
| 510 MPa @Temperature 24.0 °C, Time 360 sec |
Modulus of Elasticity | 10400 ksi |
Poissons Ratio | 0.33 |
Fracture Toughness | >= 22.0 MPa-m½ |
| >= 24.2 MPa-m½ |
| >= 26.4 MPa-m½ |
| 28.6 MPa-m½ |
| 29.7 MPa-m½ |
| 35.2 MPa-m½ |
Shear Modulus | 26.9 GPa |
Shear Strength | 44.0 ksi |
|
Electrical Properties | Original Value | Comments |
---|
Electrical Resistivity | 0.00000430 ohm-cm |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear | 12.8 µin/in-°F @Temperature 20.0 - 100 °C |
| 21.7 µm/m-°C @Temperature -50.0 - 20.0 °C |
| 23.5 µm/m-°C @Temperature 20.0 - 100 °C |
| 24.4 µm/m-°C @Temperature 20.0 - 200 °C |
| 25.4 µm/m-°C @Temperature 20.0 - 300 °C |
Specific Heat Capacity | 0.860 J/g-°C |
Thermal Conductivity | 157 W/m-K |
Melting Point | 910 - 1165 °F |
Solidus | 910 °F |
Liquidus | 1165 °F |
|
Processing Properties | Original Value | Comments |
---|
Annealing Temperature | 775 °F |
Solution Temperature | 890 °F |
Aging Temperature | 250 - 350 °F |
|
Component Elements Properties | Original Value | Comments |
---|
Aluminum, Al | 87.3 - 90.3 % |
Chromium, Cr | <= 0.04 % |
Copper, Cu | 2.0 - 2.6 % |
Iron, Fe | <= 0.15 % |
Magnesium, Mg | 1.9 - 2.6 % |
Manganese, Mn | <= 0.10 % |
Other, each | <= 0.05 % |
Other, total | <= 0.15 % |
Silicon, Si | <= 0.12 % |
Titanium, Ti | <= 0.06 % |
Zinc, Zn | 5.7 - 6.7 % |