MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Teknor Apex Sarlink® TPE EE-2270B-01 BLACK Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Sarlink EE-2270B-01 BLACK is a general purpose thermoplastic elastomer designed for automotive applications, including exterior extrusion components. Sarlink EE-2270B-01 BLACK is a medium hardness, low density, filled grade with good UV resistance designed for extrusion.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Filled; Light Stabilized; Low Density; Low Flow; Low Specific Gravity; Lubricated; Medium Hardness; Slip; Sunlight Resistant; UV Absorbing

Uses: Automotive Applications; Automotive Exterior Parts; Automotive Exterior Trim; Automotive Interior Parts; Grommets; Weatherstripping

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Extrusion

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.920 g/ccISO 1183
Viscosity 244 cP
@Shear Rate 206 1/s,
Temperature 200 °C
ASTM D3835
Melt Flow 5.0 g/10 min
@Load 5.00 kg,
Temperature 200 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 67
@Time 15.0 sec
Injection Molded; ISO 868
 68
@Time 5.00 sec
Injection Molded; ISO 868
 72
@Time 1.00 sec
Injection Molded; ISO 868
 70.3
@Treatment Temp. 125 °C,
Time 15.0 sec
Change in Air, 168 hr; ISO 888
 71.9
@Treatment Temp. 110 °C,
Time 15.0 sec
Change in Air, 1008 hr; ISO 888
 72
@Treatment Temp. 125 °C,
Time 5.00 sec
Change in Air, 168 hr; ISO 888
 74.4
@Treatment Temp. 110 °C,
Time 5.00 sec
Change in Air, 1008 hr; ISO 888
 76.4
@Treatment Temp. 125 °C,
Time 1.00 sec
Change in Air, 168 hr; ISO 888
 78.1
@Treatment Temp. 110 °C,
Time 1.00 sec
Change in Air, 1008 hr; ISO 888
Tensile Strength at Break 1120 psiFlow, Type 1, 20 in/min; ISO 37
 1540 psiAcross Flow, Type 1, 20 in/min; ISO 37
 1210 psi
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Flow, Type 1, Change in Air; ISO 188
 1230 psi
@Treatment Temp. 125 °C,
Time 605000 sec
Flow, Type 1, Change in Air; ISO 188
 1710 psi
@Treatment Temp. 125 °C,
Time 605000 sec
Across Flow, Type 1, Change in Air; ISO 188
 1740 psi
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Across Flow, Type 1, Change in Air; ISO 188
Tensile Stress at Strain 306 psi
@Strain 100 %
Across Flow, Type 1, 20 in/min; ISO 37
 403 psi
@Strain 100 %
Flow, Type 1, 20 in/min; ISO 37
 303 psi
@Strain 100 %,
Treatment Temp. 125 °C
Across Flow, Type 1, Change in Air, 168 hr; ISO 188
 317 psi
@Strain 100 %,
Treatment Temp. 110 °C
Across Flow, Type 1, Change in Air, 1008 hr; ISO 188
 387 psi
@Strain 100 %,
Treatment Temp. 125 °C
Flow, Type 1, Change in Air, 168 hr; ISO 188
 401 psi
@Strain 100 %,
Treatment Temp. 110 °C
Flow, Type 1, Change in Air, 1008 hr; ISO 188
Elongation at Break 610 %Flow, Type 1, 20 in/min; ISO 37
 770 %Across Flow, Type 1, 20 in/min; ISO 37
 590 %
@Treatment Temp. 125 °C,
Time 605000 sec
Flow, Type 1, Change in Air; ISO 188
 610 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Flow, Type 1, Change in Air; ISO 188
 740 %
@Treatment Temp. 125 °C,
Time 605000 sec
Across Flow, Type 1, Change in Air; ISO 188
 758 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Across Flow, Type 1, Change in Air; ISO 188
Tear Strength 200 pliAcross Flow; ISO 34-1
 210 pliFlow; ISO 34-1
Compression Set 24 %
@Temperature 22.8 °C,
Time 79200 sec
Type A; ISO 815
 52 %
@Temperature 70.0 °C,
Time 79200 sec
Type A; ISO 815
 65 %
@Temperature 90.0 °C,
Time 252000 sec
Type A; ISO 815
 81 %
@Temperature 125 °C,
Time 252000 sec
Type A; ISO 815
 
Processing PropertiesOriginal ValueComments
Processing Temperature 420 - 440 °FMelt, Injection
Rear Barrel Temperature 390 - 410 °FInjection
Middle Barrel Temperature 400 - 420 °FInjection
Front Barrel Temperature 410 - 430 °FInjection
Nozzle Temperature 420 - 440 °FInjection
Zone 1 380 - 400 °FExtrusion
Zone 2 390 - 410 °FExtrusion
Zone 3 400 - 420 °FExtrusion
Zone 4 400 - 420 °FExtrusion
Zone 5 410 - 430 °FExtrusion
Die Temperature 420 - 440 °FExtrusion
Mold Temperature 95.0 - 150 °FInjection
Injection Pressure 200 - 1000 psiInjection
Back Pressure 25.0 - 125 psiInjection
Cushion 0.150 - 1.00 inInjection
Screw Speed 30 - 100 rpmExtrusion
 50 - 120 rpmInjection
 
Descriptive Properties
AppearanceBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PTEKNQ1032 / 237523

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.