MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Ovako 22NiCrMo12-5* 253R Steel
Categories: Metal; Ferrous Metal; Alloy Steel; AISI 9000 Series Steel

Material Notes: General Information: Ovako 253 is a group of carburizing steel with high hardenability. High strength combined with excellent toughness and high fatigue strength makes them well suited for applications in the mining industry. Tight alloying windows provides the grades with excellent hardenability and strength control. Can be delivered as rolled, annealed normal-ized or quenched and tempered.
253A - Standard variant with high hardenability and controlled sulphur content for improved machinability.
253R - Variant with reduced sulphur content to meet the clean steel BQ (Bearing Quality) requirement for improved fatigue properties.
253L - Variant with increased carbon range for increased core hardness after carburizing. Controlled sulphur content for improved machinability.
253S - Variant with slightly increased carbon range for increased core hardness after carburizing. Controlled sulphur content for improved machinability.
4722 - Continous cast variant with slightly increased carbon range for increased hardness after carburizing.

BQ-SteelBQ-steel® is a bearing quality clean steel optimized for fatigue strength and is also ideal for new design solutions outside the bearing industry.

Information provided by Ovako

Key Words: 9317, 14NiCrMo13-4, 23NiCrMo12-5, 25NiCrMo12-5, 19NiCrMo11-5, EN27
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.80 g/cc
 
Mechanical PropertiesOriginal ValueComments
Modulus of Elasticity 210 GPa
Poissons Ratio 0.30
Shear Modulus 80.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000200 - 0.00000250 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.0 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.460 - 0.480 J/g-°C
@Temperature 50.0 - 100 °C
Thermal Conductivity 40.0 - 45.0 W/m-KAmbient temperature
Transformation Temperature 356 °CMS
 696 °CAC1
 787 °CAC3
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.22 - 0.24 %
Chromium, Cr 1.27 - 1.35 %
Iron, Fe 93.97 - 94.54 %As Balance
Manganese, Mn 0.70 - 0.75 %
Molybdenum, Mo 0.22 - 0.26 %
Nickel, Ni 2.85 - 3.05 %
Phosphorus, P <= 0.025 %
Silicon, Si 0.20 - 0.35 %
Sulfur, S 0.0050 - 0.0080 %
 
Descriptive Properties
WeldabilityCEV 0.93max
 Pcm 0.45max

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Sandvik Osprey 415 Low Alloy Steel Powder (Grade 95% - 16)

NOVAKO178 / 234477

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.