MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
SABIC LEXAN™ Copolymer EXL1444 Polycarbonate (PC) (Asia)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: Lexan* EXL1444 polycarbonate (PC) siloxane copolymer resin is a medium flow opaque injection molding (IM) grade suitable for FDA compliant applications. This resin offers extreme low temperature (-40°C) ductility, exhibits excellent processability and release with opportunities for shorter IM cycle times compared to standard PC. Lexan EXL1444 resin is a product available in wide range of opaque colors and may be an excellent candidate for a wide variety of food contact applications.

Features: High Impact Resistance

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.18 g/ccASTM D792
Density 1.19 g/ccISO 1183
Moisture Absorption 0.0200 %Injection Molding
 0.150 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 0.35 %ISO 62-1
Viscosity 9.0 cP
@Load 1.20 kg,
Temperature 300 °C
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0040 - 0.0080 cm/cmSABIC method
 0.0040 - 0.0080 cm/cm
@Thickness 3.20 mm
SABIC method
Linear Mold Shrinkage, Transverse 0.0040 - 0.0080 cm/cm
@Thickness 3.20 mm
SABIC method
Melt Flow 10 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell L 89ASTM D785
Hardness, Rockwell R 121ASTM D785
Tensile Strength at Break 50.0 MPa50 mm/min; ASTM D638
 60.0 MPa50 mm/min; ISO 527
Tensile Strength, Yield 55.0 MPa50 mm/min; ASTM D638
 57.0 MPa50 mm/min; ISO 527
Elongation at Break 98 %50 mm/min; ASTM D638
 120 %50 mm/min; ISO 527
Elongation at Yield 6.0 %50 mm/min; ASTM D638
 6.0 %50 mm/min; ISO 527
Tensile Modulus 2020 MPa50 mm/min; ASTM D638
 2150 MPa1 mm/min; ISO 527
Flexural Strength 85.0 MPayield, 2 mm/min; ISO 178
 92.0 MPayld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2230 MPa1.3 mm/min, 50 mm span; ASTM D790
 2250 MPa2 mm/min; ISO 178
Izod Impact Notched 865 JASTM D256
 775 J
@Temperature -30.0 °C
ASTM D256
Izod Impact, Notched (ISO) 70.0 kJ/m²80*10*3; ISO 180/1A
 60.0 kJ/m²
@Temperature -30.0 °C
80*10*3; ISO 180/1A
Izod Impact, Unnotched (ISO) NB80*10*3; ISO 180/1U
 NB
@Temperature -30.0 °C
80*10*3; ISO 180/1U
Charpy Impact Unnotched NBEdgew 80*10*3 sp=62mm; ISO 179/1eU
 NB
@Temperature -30.0 °C
Edgew 80*10*3 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 70.0 kJ/m²Edgew 80*10*3 sp=62mm; ISO 179/1eA
 65.0 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*3 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 70.0 JASTM D3763
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmASTM D257
Surface Resistance >= 1.00e+15 ohmASTM D257
Dielectric Constant 2.64
@Frequency 1e+6 Hz
ASTM D150
 2.68
@Frequency 100 Hz
ASTM D150
Dielectric Strength 16.3 kV/mm
@Thickness 0.800 mm
in oil; ASTM D149
Dissipation Factor 0.0012
@Frequency 100 Hz
ASTM D150
 0.0093
@Frequency 1e+6 Hz
ASTM D150
Comparative Tracking Index 175 - 250 VUL 746A
Hot Wire Ignition, HWI >= 120 sec
@Thickness >=0.700 mm
UL 746A
High Amp Arc Ignition, HAI 60 - 120 arcs
@Thickness >=0.700 mm
UL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 69.7 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 72.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 72.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
 74.7 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
Hot Ball Pressure Test 125 °CPASS; IEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 140 °CEdgew 120*10*4 sp=100mm; ISO 75/Be
 140 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 128 °CEdgew 120*10*4 sp=100mm; ISO 75/Ae
 124 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 145 °CRate B/50; ISO 306
 145 °CRate B/50; ASTM D1525
 146 °CRate B/120; ISO 306
UL RTI, Electrical 130 °CUL 746B
UL RTI, Mechanical with Impact 120 °CUL 746B
UL RTI, Mechanical without Impact 130 °CUL 746B
Flammability, UL94 HB
@Thickness >=0.700 mm
UL 94
Oxygen Index 37 %ISO 4589
Glow Wire Flammability Index 960 °C
@Thickness 1.00 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 290 - 310 °C
Zone 2 280 - 305 °C
Zone 3 295 - 315 °C
Melt Temperature 295 - 315 °CInjection Molding
Mold Temperature 70.0 - 95.0 °C
Drying Temperature 120 °CInjection Molding
Dry Time 3.00 - 4.00 hourInjection Molding
 48.0 hourCumulative; Injection Molding
Back Pressure 0.300 - 0.700 MPa
Shot Size 40 - 60 %
Vent Depth 0.00250 - 0.00760 cm
Screw Speed 40 - 70 rpm
 
Descriptive Properties
UV-light, water exposure/immersionF1UL 746C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH80176 / 288123

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.