Physical Properties | Original Value | Comments |
---|
Density | 7.65 g/cc |
Thickness | 9.00 mil |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Knoop | 167 |
Hardness, Rockwell B | 81 |
Tensile Strength, Ultimate | 51000 psi |
Tensile Strength, Yield | 48000 psi |
Elongation at Break | 9.0 % |
Modulus of Elasticity | 122 GPa |
| 143 GPa |
| 200 GPa |
| 236 GPa |
| 258 GPa |
|
Electrical Properties | Original Value | Comments |
---|
Exciting Power (RMS) | 0.00413 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00458 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00504 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00566 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.0139 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0152 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0171 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0186 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0279 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0300 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0343 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0369 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0449 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0479 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0555 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0592 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0645 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0683 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0799 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0846 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0862 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0910 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.107 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.110 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.113 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.116 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.136 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.137 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.143 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.144 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.165 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.170 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.173 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.179 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.196 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.206 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.207 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.217 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.232 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.244 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.246 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.259 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.274 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.288 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.291 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.306 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.325 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.343 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.343 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.360 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.392 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.406 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.410 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.429 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.489 RMS VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.494 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.511 RMS AT/cm @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.521 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.612 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.645 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.683 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.687 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.839 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.843 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 1.17 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.20 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 1.41 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.45 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 3.19 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 3.24 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 3.84 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 3.90 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 11.7 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 14.1 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
| 14.7 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 17.7 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
Electrical Resistivity | 0.0000510 ohm-cm |
|
Magnetic Properties | Original Value | Comments |
---|
Core Loss | 0.00147 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00154 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00192 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00201 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00257 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.00581 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.00702 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.00762 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0125 W/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0127 W/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0163 W/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0167 W/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0218 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0222 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0285 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0291 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0336 W/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0343 W/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0438 W/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0447 W/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0477 W/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0489 W/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0621 W/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0636 W/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0641 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.0659 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.0829 W/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.0834 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.0854 W/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.0858 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.104 W/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.107 W/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.108 W/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.111 W/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.128 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.132 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.135 W/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.140 W/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.154 W/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.159 W/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.166 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.172 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.183 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.189 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.200 W/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.207 W/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.217 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.223 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.238 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.246 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.255 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.263 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.282 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.291 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.303 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.304 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.311 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.331 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| <= 0.340 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.341 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.363 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.374 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.393 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.394 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.402 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| <= 0.445 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.455 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.457 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.467 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.468 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.481 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| <= 0.530 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.581 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.585 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.598 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.609 W/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 0.631 W/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| <= 0.700 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.773 W/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 0.795 W/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 0.801 W/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 0.824 W/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 0.999 W/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
| 1.03 W/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
|
Descriptive Properties |
---|
Magnetostriction 10^8 | -80 |
| -94 |
Minimum Lamination Factor (%) | 94.5 |
Minimum Peak Permeability at 10 Oe | 1780 |
Typical Lamination Factor (%) | 96.1 |
Typical Peak Permeability at 10 Oe | 1844 |