MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Syensqo (Solvay Specialty Polymers) KetaSpire® KT-820 NL PEEK, Low melt flow for extrusion and injection molding
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK)

Material Notes: Low melt flow for extrusion and injection molding, not lubricated

KetaSpire® KT-820 NL is a low flow grade of unreinforced polyetheretherketone (PEEK) supplied in non-lubricated, natural-color pellet form. KetaSpire® PEEK is produced to the highest industry standards and is characterized by a distinct combination of properties, which include excellent wear resistance, best-in-class fatigue resistance, ease of melt processing, high purity, and excellent chemical resistance to organics, acids, and bases.

These properties make it well-suited for applications in healthcare, transportation, electronics, chemical processing, and other industrial uses.

This resin is also available as KetaSpire® KT-820P in a natural-color coarse powder form for compounding.

A lubricated form of the resin is available as KT-820 in either natural (NT) or black (BK 95). The lubricated version is lightly dusted with calcium stearate (0.01% level) to aid with pellet conveyance in plastication screws.

Applications: Aircraft Applications; Automotive Applications; Electrical/Electronic Applications; Film; Industrial Applications; Medical/Healthcare Applications; Oil/Gas Applications

Features: Chemical Resistant; Ductile; Fatigue Resistant; Flame Retardant; Good Dimensional Stability; Good Impact Resistance; High Heat Resistance

Standard Packaging and Labeling
- KetaSpire resins are packaged in polyethylene buckets or cardboard boxes depending upon the order size. Individual packages will be plainly marked with the product, color, lot number, and net weight.

Injection notes: Drying
- KetaSpire resins must be dried completely prior to melt processing. Incomplete drying will result in defects in the formed part ranging from surface streaks to severe bubbling. Pellets can be dried on trays in a circulating air oven or in desiccating hopper dryer. Drying conditions recommended are 4 hours at 150°C (300°F) .
Injection Molding
- KetaSpire resins can be readily injection molded in most screw injection machines. A general purpose screw with a compression ratio in the range of 2.5 - 3.5 : 1 is recommended, as is minimum back pressure. Injection speeds should be as fast as possible, consistent with part appearance requirements. Mold temperatures in the range of 175°C to 205°C (350°F to 400°F) are suggested. Recommended starting point barrel temperatures are shown in the following table.

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.30 g/ccASTM D792
Water Absorption 0.10 %
@Time 86400 sec
ASTM D570
Linear Mold Shrinkage, Flow 0.015 cm/cmASTM D955
Linear Mold Shrinkage, Transverse 0.018 cm/cmASTM D955
Melt Flow 3.0 g/10 min
@Load 2.16 kg,
Temperature 400 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 88
@Time 1.00 sec
ASTM D2240
Tensile Strength 95.0 MPa50 mm/min; ASTM D638
Tensile Strength, Yield 96.0 MPaType 1A, 50 mm/min; ISO 527-2
Elongation at Break 20 - 30 %50 mm/min; ASTM D638
 20 - 30 %Type 1A, 50 mm/min; ISO 527-2
Elongation at Yield 4.9 %Type 1A, 50 mm/min; ISO 527-2
 5.2 %50 mm/min; ASTM D638
Tensile Modulus 3500 MPa50 mm/min; ASTM D638
 3830 MPa1 mm/min, Type 1A; ISO 527-2
Flexural Strength 146 MPaASTM D790
Flexural Modulus 3700 MPaASTM D790
Izod Impact, Notched 91.0 J/mASTM D256
Izod Impact, Unnotched NBASTM D256
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 43.0 µm/m-°C
@Temperature -50.0 - 50.0 °C
ASTM E831
Melting Point 340 °CPeak; ASTM D3418
Deflection Temperature at 1.8 MPa (264 psi) 157 °CUnannealed; ASTM D648
Glass Transition Temp, Tg 150 °CDSC
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 355 °C
Middle Barrel Temperature 365 °C
Front Barrel Temperature 370 °C
Nozzle Temperature 375 °C
Mold Temperature 175 - 205 °C
Drying Temperature 150 °C
@Time 14400 sec
 
Descriptive Properties
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
ColorNatural Color
FormsPellets
Injection RateFast
ProcessingInjection Molding; Machining; Profile Extrusion
RoHS ComplianceYes
Screw Compression Ratio2.5:1.0 to 3.5:1.0

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSOL8Y4320 / 280120

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.