MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Gougeon Brothers PRO-SET® M1002/M2046 Laminating Epoxy
Categories: Polymer; Thermoset; Epoxy

Material Notes: Medium viscosity for good wet out of all synthetic composite fabrics and core materials.
Slow cure speed hardener provides 4.5 to 6 hours of working time at 72°F (22°C).
Elevated temperature cure is required; thermal and mechanical properties suitable for composite components and high temperature tooling and molds.
Tg as high as 197°F (92°C) with proper post cure providing excellent temperature stability and great part cosmetics.
Cost effective, high performance epoxy formulation for synthetic composite manufacturing.
Quality-control tinting is available at no extra charge; simply add "QC" after the product code on your order.

Information provided by Gougeon Brothers, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.17 g/ccCured
Viscosity 115 cPhardener; ASTM D2196
 2100 cPMixed; ASTM D2196
 4800 cPresin; ASTM D2196
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 83
@Treatment Temp. 22.0 °C,
Time 1.21e+6 sec
ASTM D2240
 83
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D2240
Tensile Strength 1000 psi
@Treatment Temp. 22.0 °C,
Time 1.21e+6 sec
ASTM D638
 9590 psi
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D638
Elongation at Break 5.5 %
@Treatment Temp. 22.0 °C,
Time 1.21e+6 sec
ASTM D638
 5.7 %
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D638
Tensile Modulus 394000 psiRT Gelation; ASTM D638
 433000 psiASTM D638
Flexural Strength 17700 psi
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D790
 18800 psi
@Treatment Temp. 22.0 °C,
Time 1.21e+6 sec
ASTM D790
Flexural Modulus 514000 psi
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D790
 555000 psi
@Treatment Temp. 22.0 °C,
Time 1.21e+6 sec
ASTM D790
Compressive Yield Strength 13900 psi
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D695
 14100 psi
@Treatment Temp. 22.0 °C,
Time 1.21e+6 sec
ASTM D695
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 170 °F
@Treatment Temp. 22.0 °C,
Time 1.21e+6 sec
ASTM D648
 189 °F
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D648
Glass Transition Temp, Tg 197 °FASTM E1356
 176 °F
@Treatment Temp. 22.0 °C,
Time 1.21e+6 sec
DSC Onset– 1st Heat, RT Gelation; ASTM E1356
 197 °F
@Treatment Temp. 60.0 °C,
Time 28800 sec
DSC Onset– 1st Heat, RT Gelation; ASTM E1356
 
Processing PropertiesOriginal ValueComments
Pot Life 72.0 - 88.0 min
@Load 0.100 kg
ASTM D2471
Working Life 4.50 - 6.00 hour
Shelf Life 18.0 Monthhardener
 36.0 Monthresin
 
Descriptive Properties
Mix ratio100:24Weight, Resin: Hardener
 100:26.10–100:20.90Weight Range, Resin: Hardener
 100:28Volume, Resin: Hardener
 100:31.60–100:25.30Volume Range, Resin: Hardener
 3.16:1–3.95:1Volume Range, Resin: Hardener
 3.57:1Volume, Resin: Hardener
 3.83:1–4.78:1Weight Range, Resin: Hardener
 4.17:1Weight, Resin: Hardener

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PGOUGP927 / 290770

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.