MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Teknor Apex Sarlink® TPE ML-1640N NA Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Sarlink ML-1600 is a high performance, high flow thermoplastic elastomer series, available in NAT and BLK designed for automotive interior applications. Sarlink ML-1640N NAT is a low hardness, medium density grade with excellent surface appearance suitable for injection molding.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; Filled; Good Adhesion; Good Flexibility; Good Moldability; Good Processability; Good Surface Finish; Good Tear Strength; Good Toughness; High Flow; Medium Density; Low Hardness; Resilient

Uses: Automotive Applications; Automotive Interior Parts; Flexible Grips; Grommets; Knobs; Rubber Replacement; Soft Touch Applications

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding

Preliminary data. Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.00 g/ccISO 1183
Viscosity 122 cP
@Shear Rate 206 1/s,
Temperature 200 °C
ASTM D3835
Melt Flow 6.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 39
@Time 15.0 sec
Injection Molded; ISO 868
 41
@Time 5.00 sec
Injection Molded; ISO 868
 43
@Time 1.00 sec
Injection Molded; ISO 868
 39.3
@Treatment Temp. 110 °C,
Time 15.0 sec
Change in Air, 1008 hr; ISO 888
 39.9
@Treatment Temp. 125 °C,
Time 15.0 sec
Change in Air, 168 hr; ISO 888
 42.4
@Treatment Temp. 125 °C,
Time 5.00 sec
Change in Air, 168 hr; ISO 888
 44
@Treatment Temp. 110 °C,
Time 5.00 sec
Change in Air, 1008 hr; ISO 888
 44.8
@Treatment Temp. 125 °C,
Time 1.00 sec
Change in Air, 168 hr; ISO 888
 45.5
@Treatment Temp. 110 °C,
Time 1.00 sec
Change in Air, 1008 hr; ISO 888
Tensile Strength at Break 624 psiFlow, Type 1, 20 in/min; ISO 37
 827 psiAcross Flow, Type 1, 20 in/min; ISO 37
 830 psi
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Flow, Type 1, Change in Air; ISO 188
 830 psi
@Treatment Temp. 125 °C,
Time 605000 sec
Flow, Type 1, Change in Air; ISO 188
 1010 psi
@Treatment Temp. 125 °C,
Time 605000 sec
Across Flow, Type 1, Change in Air; ISO 188
 1020 psi
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Across Flow, Type 1, Change in Air; ISO 188
Tensile Stress at Strain 122 psi
@Strain 100 %
Across Flow, Type 1, 20 in/min; ISO 37
 183 psi
@Strain 100 %
Flow, Type 1, 20 in/min; ISO 37
 123 psi
@Strain 100 %,
Treatment Temp. 110 °C
Across Flow, Type 1, Change in Air, 1008 hr; ISO 188
 125 psi
@Strain 100 %,
Treatment Temp. 125 °C
Across Flow, Type 1, Change in Air, 6.61 in; ISO 188
 188 psi
@Strain 100 %,
Treatment Temp. 110 °C
Flow, Type 1, Change in Air, 1008 hr; ISO 188
 197 psi
@Strain 100 %,
Treatment Temp. 125 °C
Flow, Type 1, Change in Air, 168 hr; ISO 188
Elongation at Break 820 %Flow, Type 1, 20 in/min; ISO 37
 980 %Across Flow, Type 1, 20 in/min; ISO 37
 943 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Flow, Type 1, Change in Air; ISO 188
 968 %
@Treatment Temp. 125 °C,
Time 605000 sec
Flow, Type 1, Change in Air; ISO 188
 1090 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Across Flow, Type 1, Change in Air; ISO 188
 1240 %
@Treatment Temp. 125 °C,
Time 605000 sec
Across Flow, Type 1, Change in Air; ISO 188
Tear Strength 89.0 pliAcross Flow, Method Ba, Angle (Unnicked), 20 in/min; ISO 34-1
 100 pliFlow, Method Ba, Angle (Unnicked), 20 in/min; ISO 34-1
Compression Set 16 %
@Temperature 22.8 °C,
Time 79200 sec
Type 1; ISO 815
 33 %
@Temperature 70.0 °C,
Time 79200 sec
Type 1; ISO 815
 61 %
@Temperature 90.0 °C,
Time 252000 sec
Type 1; ISO 815
 90 %
@Temperature 125 °C,
Time 252000 sec
Type 1; ISO 815
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 340 - 380 °F
Middle Barrel Temperature 350 - 390 °F
Front Barrel Temperature 360 - 400 °F
Nozzle Temperature 370 - 410 °F
Melt Temperature 370 - 410 °F
Mold Temperature 77.0 - 150 °F
Injection Pressure 200 - 1000 psi
Back Pressure 25.0 - 50.0 psi
Cushion 0.150 - 1.00 in
Screw Speed 50 - 100 rpm
 
Descriptive Properties
AppearanceNatural Color

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PTEKNQ1107 / 237598

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.