MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Materion Beryllium Oxide, BeO >99.5%
Categories: Ceramic; Oxide

Material Notes: Isopressed Ceramic CDI-20, Rev E

Information provided by Materion.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.85 g/ccASTM C-373-88
Grain Size 9.00 - 25.0 µmASTM E-112-96
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell 45 N >= 60.0ASTM E-18-96
Tensile Strength 22.0 ksiASTM C-565-93
Modulus of Elasticity 50000 ksiASTM C-623-92
Flexural Strength 221 MPaASTM F-417-78
Compressive Strength 1550 MPaASTM C-773-88
Poissons Ratio 0.260ASTM C-565-93
Shear Modulus 19800 ksiCalculated
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmASTM D-257-93
Dielectric Constant 6.67
@Frequency 9.30e+9 Hz
ASTM D-2520-95
 6.73
@Frequency 1.00e+6 Hz
ASTM D-150-95
Dielectric Strength 230 V/mil
@Thickness 6.35 mm
ASTM D-116-86
Dissipation Factor <= 0.000400
@Frequency 1.00e+6 Hz
ASTM D-150-95
 <= 0.000400
@Frequency 9.30e+9 Hz
ASTM D-2520-95
 
Thermal PropertiesOriginal ValueComments
CTE, linear 5.00 µin/in-°F
@Temperature 25.0 - 1000 °C
ASTM E-228-95
Specific Heat Capacity 1.05 J/g-°CASTM C-351-92b
Thermal Conductivity 150 W/m-K
@Temperature 150 °C
Axial Rod Method (Ref ASTM C-408-88); ASTM E-228-95
 180 W/m-K
@Temperature 150 °C
Laser Flash Method; ASTM E-228-95
 188 W/m-K
@Temperature 100 °C
Axial Rod Method (Ref ASTM C-408-88); ASTM E-228-95
 220 W/m-K
@Temperature 100 °C
Laser Flash Method; ASTM E-228-95
 251 W/m-K
@Temperature 25.0 °C
Axial Rod Method (Ref ASTM C-408-88); ASTM E-228-95
 285 W/m-K
@Temperature 25.0 °C
Laser Flash Method; ASTM E-228-95
 
Component Elements PropertiesOriginal ValueComments
BeO >= 99.5 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

CMATER907 / 323519

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.