MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
LyondellBasell Petrothene GA501152 Linear Low Density Polyethylene (LLDPE), Film Grade
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Film Grade

Material Notes: The Petrothene GA501 series of resins is pelletized liner low density polyethylene selected for film extrusion applications that require excellent drawdown and toughness. These resins have excellent puncture resistance, elongation and heat seal strength. Typical applications include heavy duty shipping sacks, trash can liners, commercial and industrial packaging, as well as food and consumer packaging. GA501 is available without additives or fully formulated with slip and antiblock additives. Applications: Agriculture Film, Bags & Pouches, Can Liners, Film Wrap, Food Packaging Film, Heavy Duty Packaging, Lamination Film, Liner Film, Retail Carryout Bags, Shrink Film.

Information provided by LyondellBasell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Base Resin Density 0.918 g/ccASTM D1505
Density 0.925 g/ccASTM D1505
Melt Flow 1.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
Antiblock Level 10000 ppmLYB Method
Slip Level 1000 ppmLYB Method
 
Mechanical PropertiesOriginal ValueComments
Film Elongation at Break, MD 580 %ASTM D882
Film Elongation at Break, TD 725 %ASTM D882
Elmendorf Tear Strength MD 125 gASTM D1922
Elmendorf Tear Strength TD 330 gASTM D1922
Dart Drop Test 100 gF50; ASTM D1709
Film Tensile Strength at Break, MD 45.5 MPaASTM D882
Film Tensile Strength at Break, TD 32.4 MPaASTM D882
1% Secant Modulus, MD 186 MPaASTM D882
1% Secant Modulus, TD 193 MPaASTM D882
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 107 °CASTM D1525
 
Processing PropertiesOriginal ValueComments
Melt Temperature 400 - 450 °F1.5 to 3.0:1 blow up ratio
 
Descriptive Properties
Polymer Processing AidPresent, LYB Method
Processing MethodBlown Film
Test Specimen1.0 mil gauge, 2.5:1 BUR

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Total Lumicene® mPE M 2735 S01 Metallocene Polyethylene, Cast Film
Total Lotrene® Q2018N Linear Low Density Polyethylene, Cast Film
Total Lotrene® Q2018H Linear Low Density Polyethylene, Blown Film
Total Lotrene® Q1018H Linear Low Density Polyethylene, Blown Film
Total LLDPE LL 1820 Linear Low Density Polyethylene - Blown Film

PEQT8819 / 220453

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.