MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Covestro Baydur® GS PUR Polyurethane  (discontinued **)
Categories: Polymer; Thermoset; Polyurethane, TS; Thermoset Polyurethane, Liquid

Material Notes: Polyurethane casting system for the production of solid components. Pressureless casting into open or closed molds, fast demold times, good rot resistance. Combines easily with other materials.

Information provided by Bayer.

As of 1 September 2015, Bayer MaterialScience was separated from Bayer AG and officially adopted its new name – Covestro.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.17 g/cc
Water Absorption at Saturation 3.3 %
 3.3 %
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 45.0 MPa
Elongation at Break 23 %
Tensile Modulus 1.30 GPa
Charpy Impact Unnotched 6.00 J/cm²
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 9.00e+13 ohm-cm
Surface Resistance 1.00e+13 ohm
Dielectric Strength 15.0 kV/mm
Comparative Tracking Index 600 V
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 135 µm/m-°C
@Temperature 20.0 °C
CTE, linear, Transverse to Flow 135 µm/m-°C
@Temperature 20.0 °C
Deflection Temperature at 0.46 MPa (66 psi) 67.0 °C
Deflection Temperature at 1.8 MPa (264 psi) 55.0 °C
Vicat Softening Point 94.0 °C

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 5154-H112
North American Northern Red Oak Wood
Covestro Baydur® GS-772 Polyurethane Solid RIM, MDI-based 2-Component Liquid System
Covestro Baydur® 646 Polyurethane Structural Foam RIM, Density 20 pcf, MDI-based 2-Component Liquid System
Covestro Baydur® 646 Polyurethane Structural Foam RIM, Density 25 pcf, MDI-based 2-Component Liquid System

PBA080 / 26690

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.