MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
NYCOA 5033 HS 33% Glass-Fiber Reinforced, Heat Stabilized, Nylon 66 Resin
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled

Material Notes: NYCOA 5033 HS is a 33% glass fiber reinforced, heat stabilized Nylon 66 resin used for injection molding. It offers an outstanding balance of mechanical properties over standard grades of conventional Nylon 66.

NYCOA 5033 HS has been specifically formulated for optimum thermal stability and chemical resistance.

This grade is available in UV stable, custom colors, and impact modified grades. Typical applications include pedal brackets and supports, air intake manifolds, radiator end tanks, valve covers, and power tool housings.

Information provided by Nycoa, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.38 g/ccASTM D792
Water Absorption 0.70 %24 hours; ASTM D570
Linear Mold Shrinkage 0.0050 cm/cmASTM D955
Linear Mold Shrinkage, Transverse 0.0080 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 122ASTM D785
Tensile Strength, Yield 200 MPaASTM D638
Elongation at Break 4.0 %ASTM D638
Flexural Strength 260 MPaASTM D790
Flexural Modulus 8.90 GPaASTM D790
Izod Impact, Notched 130 J/mASTM D256
 
Thermal PropertiesOriginal ValueComments
Melting Point 263 °CASTM D789
Deflection Temperature at 0.46 MPa (66 psi) 260 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 240 °CASTM D648

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
NYCOA 2084 HS PA 6
NYCOA 534H PA 6
NYCOA 715C PA 6
NYCOA 2084 HS Super-Tough, High Viscosity Nylon 6 Resin
NYCOA 400 PA 6

PNYCO03 / 55538

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.