MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Morgan Advanced Ceramics Vitox® AMC Alumina Matrix Composite Aluminum Oxide Ceramic
Categories: Ceramic; Ceramic Matrix Composite; Oxide; Aluminum Oxide

Material Notes: A very high purity, sub-micron grain sized zirconia toughened alumina matrix composite ceramic. Composed of a 99.9% alumina and 3mol% yttria partially stabilized zirconia (Y-PSZ), produced specifically for surgical implant devices.

Prime Features:

  • Ultra-fine sub-micron grain size
  • Homogeneous microstructure
  • High Mechanical strength
  • High fracture toughness
  • High levels of QA and traceability.
Typical Applications:
  • Joint replacement components
  • Femoral heads to match cup liners of same material, HIP Vitox or UHMWPE
  • Cup liners
  • Other implantable devices
Production Capabilities:
  • 26 to 60 mm head diameters with various neck length and taper options
  • Taper lock cup inserts for 28 to 72 mm heads
  • Hemispherical designs for 28 to 68 mm heads
  • Custom design femoral heads and cup inserts to OEM requirements

Information provided by Morgan Advanced Materials

Key Words: Alumina Matrix Composite
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 4.26 g/ccfired
Grain Size 0.16 µmY-PSZ, average
 0.67 µmAlumina, average
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 17
@Load 1.00 kg
[GPa]
Modulus of Elasticity 370 GPa
Flexural Strength 400 MPabiaxial
 700 MPa4-point
Fracture Toughness 4.50 MPa-m½KIC(SEVNB)
 5.70 MPa-m½KIC(Indentation)
 
Component Elements PropertiesOriginal ValueComments
Al2O3 99.9 %
 
Descriptive Properties
Colorwhite

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Morgan Advanced Ceramics Vitox® AMC Alumina Matrix Composite Technical Ceramic
COI Ceramics Sylramic™ S400 Silicon Carbide Ceramic Matrix Composite, Carbon
Silicon Carbide, Reaction-Bonded, SiSiC
M Cubed Technologies SSC-702 Reaction-Bonded Silicon Carbide
COI Ceramics Nextel™ AS-N720 Oxide Ceramic Matrix Composite, Aluminosilicate

CMORF5011 / 200249

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.