MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Schmolz + Bickenbach UGIMA® 630 Stainless Steel Bar
Categories: Metal; Ferrous Metal; Stainless Steel; Precipitation Hardening Stainless; T 600 Series Stainless Steel

Material Notes: 630 UGIMA® is an improved machining martensitic precipitation hardenable grade. It is identical to standard type 630 (17-4), except with respect to machinability. The proprietary UGIMA® manufacturing process – developed by Ugitech – results in a product that increases productivity and tool life, and improves the surface finish on all types of machined parts. 630 UGIMA® provides a good combination of high strength corrosion resistance, and is often the best solution of stainless steel when high strength is required. Parts machined from solution treated bar stock should be heat treated or aged prior to use. No further heat treatment of machined parts is required when using 630 UGIMA® is one of the precipitation hardened conditions as specified.

Applications: Fasteners, Shafts, Valve Bodies, Valves, Valve Trim, Fitting, Machined parts, Medical devices, Aircraft components, and Not recommended for vessels containing liquid or gasses at high pressure

Information provided by Schmolz + Bickenbach

Key Words: AISI 630; UNS S17400; EN 10088-3 1.4542, X5CrNiCuNB16.4; ASTM A484; A564; F899; ASME SA-564; API 6A
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.75 g/cc0.280 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell >= 277>= 2771400°F for 2 hrs and 1150°F for 4 hrs
 320 - 340
@Thickness <=25.4 mm
320 - 340
@Thickness <=1.00 in
Cold Drawn Bars
 320 - 340
@Thickness >=25.4 mm
320 - 340
@Thickness >=1.00 in
Turned Bars
 >= 255
@Treatment Temp. 579.4 °C,
Time 14400 sec
>= 255
@Treatment Temp. 1075 °F,
Time 4.00 hour
 >= 255
@Treatment Temp. 621 °C,
Time 14400 sec
>= 255
@Treatment Temp. 1150 °F,
Time 4.00 hour
 >= 331
@Treatment Temp. 551.7 °C,
Time 14400 sec
>= 331
@Treatment Temp. 1025 °F,
Time 4.00 hour
 >= 388
@Treatment Temp. 482 °C,
Time 3600 sec
>= 388
@Treatment Temp. 900 °F,
Time 1.00 hour
Tensile Strength >= 793 MPa>= 115000 psi1400°F for 2 hrs and 1150°F for 4 hrs
 1000 - 1140 MPa
@Thickness <=25.4 mm
145000 - 165000 psi
@Thickness <=1.00 in
Cold Drawn Bars
 1030 - 1170 MPa
@Thickness >=25.4 mm
150000 - 170000 psi
@Thickness >=1.00 in
Turned Bars
 >= 931 MPa
@Treatment Temp. 621 °C,
Time 14400 sec
>= 135000 psi
@Treatment Temp. 1150 °F,
Time 4.00 hour
 >= 1000 MPa
@Treatment Temp. 579.4 °C,
Time 14400 sec
>= 145000 psi
@Treatment Temp. 1075 °F,
Time 4.00 hour
 >= 1070 MPa
@Treatment Temp. 551.7 °C,
Time 14400 sec
>= 155000 psi
@Treatment Temp. 1025 °F,
Time 4.00 hour
 >= 1310 MPa
@Treatment Temp. 482 °C,
Time 3600 sec
>= 190000 psi
@Treatment Temp. 900 °F,
Time 1.00 hour
Tensile Strength, Yield >= 517 MPa>= 75000 psi1400°F for 2 hrs and 1150°F for 4 hrs
 >= 862 MPa
@Temperature 1075 °C,
Time 14400 sec
>= 125000 psi
@Temperature 1967 °F,
Time 4.00 hour
 >= 862 MPa
@Temperature 1150 °C,
Time 14400 sec
>= 125000 psi
@Temperature 2100 °F,
Time 4.00 hour
 >= 1070 MPa
@Temperature 1025 °C,
Time 14400 sec
>= 155000 psi
@Temperature 1877 °F,
Time 4.00 hour
 >= 1170 MPa
@Temperature 900 °C,
Time 3600 sec
>= 170000 psi
@Temperature 1650 °F,
Time 1.00 hour
 793 - 931 MPa
@Strain 0.2 %,
Thickness >=25.4 mm
115000 - 135000 psi
@Strain 0.2 %,
Thickness >=1.00 in
Turned Bars
 931 - 1070 MPa
@Strain 0.2 %,
Thickness <=25.4 mm
135000 - 155000 psi
@Strain 0.2 %,
Thickness <=1.00 in
Cold Drawn Bars
Elongation at Yield >= 18 %>= 18 %1400°F for 2 hrs and 1150°F for 4 hrs
 >= 0.00 %
@Thickness <=25.4 mm
>= 0.00 %
@Thickness <=1.00 in
Cold Drawn Bars
 >= 12 %
@Thickness >=25.4 mm
>= 12 %
@Thickness >=1.00 in
Turned Bars
 >= 10 %
@Treatment Temp. 482 °C,
Time 3600 sec
>= 10 %
@Treatment Temp. 900 °F,
Time 1.00 hour
 >= 12 %
@Treatment Temp. 551.7 °C,
Time 14400 sec
>= 12 %
@Treatment Temp. 1025 °F,
Time 4.00 hour
 >= 13 %
@Treatment Temp. 579.4 °C,
Time 14400 sec
>= 13 %
@Treatment Temp. 1075 °F,
Time 4.00 hour
 >= 16 %
@Treatment Temp. 621 °C,
Time 14400 sec
>= 16 %
@Treatment Temp. 1150 °F,
Time 4.00 hour
Reduction of Area >= 55 %>= 55 %1400°F for 2 hrs and 1150°F for 4 hrs
 >= 40 %
@Thickness >=25.4 mm
>= 40 %
@Thickness >=1.00 in
Turned Bars
 >= 50 %
@Thickness <=25.4 mm
>= 50 %
@Thickness <=1.00 in
Cold Drawn Bars
 >= 34 %
@Treatment Temp. 482 °C,
Time 3600 sec
>= 34 %
@Treatment Temp. 900 °F,
Time 1.00 hour
 >= 45 %
@Treatment Temp. 551.7 °C,
Time 14400 sec
>= 45 %
@Treatment Temp. 1025 °F,
Time 4.00 hour
 >= 50 %
@Treatment Temp. 579.4 °C,
Time 14400 sec
>= 50 %
@Treatment Temp. 1075 °F,
Time 4.00 hour
 >= 50 %
@Treatment Temp. 621 °C,
Time 14400 sec
>= 50 %
@Treatment Temp. 1150 °F,
Time 4.00 hour
Tensile Modulus 197 GPa28600 ksi
Charpy Impact  >= 20.3 J
@Treatment Temp. 551.7 °C,
Time 14400 sec
>= 15.0 ft-lb
@Treatment Temp. 1025 °F,
Time 4.00 hour
 >= 40.7 J
@Treatment Temp. 579.4 °C,
Time 14400 sec
>= 30.0 ft-lb
@Treatment Temp. 1075 °F,
Time 4.00 hour
 >= 40.7 J
@Treatment Temp. 621 °C,
Time 14400 sec
>= 30.0 ft-lb
@Treatment Temp. 1150 °F,
Time 4.00 hour
 >= 74.6 J
@Treatment Temp. 760 °C,
Time 7200 sec
>= 55.0 ft-lb
@Treatment Temp. 1400 °F,
Time 2.00 hour
 >= 74.6 J
@Treatment Temp. 621 °C,
Time 14400 sec
>= 55.0 ft-lb
@Treatment Temp. 1150 °F,
Time 4.00 hour
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000800 ohm-cm0.0000800 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 10.8 µm/m-°C
@Temperature 20.0 - 200 °C
6.00 µin/in-°F
@Temperature 68.0 - 392 °F
Thermal Conductivity 34.3 W/m-K
@Temperature 20.0 °C
238 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 1040 °C1900 °F
Hot-Working Temperature 801.7 °C1475 °FStep 1: Slow heating
 949 - 1200 °C1740 - 2190 °FStep 3: Forging range
 1150 - 1200 °C2100 - 2190 °FStep 2: More Rapid Heating
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.070 %<= 0.070 %
Chromium, Cr 15 - 17.5 %15 - 17.5 %
Copper, Cu 3.0 - 4.0 %3.0 - 4.0 %
Iron, Fe >= 70.46 %>= 70.46 %
Manganese, Mn <= 1.0 %<= 1.0 %
Nickel, Ni 3.0 - 5.0 %3.0 - 5.0 %
Niobium, Nb (Columbium, Cb) 0.15 - 0.45 %0.15 - 0.45 %
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %
Tantalum, Ta 0.15 - 0.45 %0.15 - 0.45 %
 
Descriptive Properties
Corrosion ResistanceAcetic Acid2/4
 Humidity4/4
 NaCl (Saline Mist)3/4
 Nitric Acid3/4
 Sodium Carbonate2/4

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Carpenter Custom 630 (17-Cr-4Ni) Precipitation Hardening Stainless Steel, Condition H 900 (Age-Hardened 482°C/1hr/AC)
AK Steel 17-4 PH® Precipitation Hardening Stainless Steel, Condition H 900
Carpenter Custom 630 (17-Cr-4Ni) Precipitation Hardening Stainless Steel, Annealed
Carpenter Custom 630 (17-Cr-4Ni) Precipitation Hardening Stainless Steel, Condition H 1025 (Heated 552°C)
AK Steel 17-4 PH® Precipitation Hardening Stainless Steel, Condition A

NSCHMO039 / 125912

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.