MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Arkema Altuglas® GR 7E LIL Acrylic  (discontinued **)
Categories: Polymer; Thermoplastic; Acrylic (PMMA); Acrylic, General Purpose, Molded

Material Notes: ALTUGLAS GR 7E LIL is an injection molding grade with excellent balance between mechanical, thermal and optical properties.

Key features :

  • easy processing and demolding
  • improved chemical resistance
  • good resistance to dishwashing cycling

ALTUGLAS GR 7E LIL is particularly recommended for houseware applications like: salad bowls, tumblers, cutlery handles and other house ware parts that require resistance to dishwasher cycling.

ISO data provided by the manufacturer, Arkema.

Arkema sold its PMMA business to Trinseo in 2021.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.18 g/cc0.0426 lb/in³
Water Absorption 1.9 %1.9 %
Moisture Absorption at Equilibrium 0.30 %0.30 %Humidity Absorption
Melt Flow 2.4 g/10 min
@Load 3.80 kg,
Temperature 230 °C
2.4 g/10 min
@Load 8.38 lb,
Temperature 446 °F
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 85.0 MPa12300 psi50 mm/min
Elongation at Break 6.0 %6.0 %Nominal Strain; 50 mm/min
Tensile Modulus 3.30 GPa479 ksi1 mm/min
Charpy Impact Unnotched 2.00 J/cm²9.52 ft-lb/in²
Charpy Impact, Notched 0.200 J/cm²0.952 ft-lb/in²
Tensile Creep Modulus, 1 hour 2700 MPa392000 psi
Tensile Creep Modulus, 1000 hours 1800 MPa261000 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cm
Surface Resistance 1.00e+14 ohm1.00e+14 ohm
Dielectric Constant  3.2
@Frequency 1e+6 Hz
3.2
@Frequency 1e+6 Hz
 3.7
@Frequency 100 Hz
3.7
@Frequency 100 Hz
Dielectric Strength 19.7 kV/mm500 kV/in
Dissipation Factor  0.040
@Frequency 1e+6 Hz
0.040
@Frequency 1e+6 Hz
 0.050
@Frequency 100 Hz
0.050
@Frequency 100 Hz
Comparative Tracking Index 600 V600 V
 
Thermal PropertiesMetricEnglishComments
CTE, linear 70.0 µm/m-°C
@Temperature 20.0 °C
38.9 µin/in-°F
@Temperature 68.0 °F
Deflection Temperature at 0.46 MPa (66 psi) 97.0 °C207 °F
Deflection Temperature at 1.8 MPa (264 psi) 92.0 °C198 °F
Vicat Softening Point 80.0 °C176 °F50°C/hr; 50N
Flammability, UL94 HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
 
Optical PropertiesMetricEnglishComments
Transmission, Visible 80 %80 %Mfr. reports 'Transparent' but doesn't quantify.

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
RTP Company RTP 1400 R-5000 Polyphenylsulfone (PPSU), Transparent
Covestro Makrolon® 2458 Polycarbonate, Injection Grade
BASF Ultrason® E 1010 PES
BASF Ultrason® E 2010 G4 MR SW 15102 20% Glass Filled PESU
BASF Ultrason® E 6020 P PES

PARKG215 / 25506

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.